If little circles open as the lacquer lands, look for a wetting problem first. If the coat looks even when sprayed and develops small bubbles or pinholes as it dries, investigate solvent pop. The holes can look much alike once the finish is dry, so note when and where they first appear.
Record which coat showed the defect and whether it is clustered at an overlap, spread across several pieces or following the grain. Those details are more useful than the finished crater alone.
Tell Solvent Pop from Fisheyes
|
What you observe |
Likely first check |
What to compare |
|
The wet film draws back into round craters |
Poor wetting around contamination |
Waxes, silicone, oil, cleaners and the spray air |
|
Small bubbles or open pinholes appear as the film sets |
Solvent escaping through a surface that has started to set |
Coat weight, flash time and drying conditions |
|
Holes come back over the same grain or substrate spots |
Porosity or an earlier layer may be involved |
The sealed substrate on a prepared comparison panel |
Timing gives you a place to start. It does not prove the cause. A contaminant can be present on both the substrate and the spray line, and you can have more than one defect on the same panel. The guide to fisheyes in automotive clear coat shows what to look for when a wet film pulls away.
Trace Solvent Pop Back to the Coat Schedule
Look at the areas where the finish went on heaviest. On a door profile, for instance, the same corner may catch material from two passes. A coat that seems even on the flat can build more at that return. Check the actual film build and the time between coats against the product data sheet (PDS). Also check whether the part went into a warm drying area too soon or the airflow changed. The PPG solvent pop guide outlines the role of trapped solvent.
Pre-catalyzed and post-catalyzed lacquers have different handling requirements. Use the instructions for the exact product, including permitted thinner, catalyst if required, film build and dry schedule. The MagnaMax product documentation is one example of a pre-catalyzed system. It is not a mixing or drying schedule for another lacquer. Keep the approved ventilation operating; do not change booth airflow, add an unapproved retarder or force dry the finish to chase the defect.
Find a Fisheye Source Before Recoating
If the wet film opens up, check what touched the piece between sanding and spraying. Cleaners, reused cloths, polish and silicone sprays can transfer residues. Trace the gun and air line too, especially if the same problem appears on different substrates or with a different batch of lacquer.
Start with the filters, water separator and connections, then the hose at the gun. A line shared with lubricated air tools is worth checking. Follow the shop's approved air-quality test, such as the ASTM compressed air blotter procedure where applicable. It screens for oil or water; a clear result does not certify that the booth or substrate is free of contamination. Replace or dedicate a hose when it is implicated rather than swapping parts at random. Review the wood finishing spray setup guide for the rest of the air and ventilation checks.
Repair the Affected Layer and Test Again
Stop adding finish and let the coating reach the manufacturer's repair stage. If a shallow defect can be leveled while leaving sound film within the approved limits, prepare and recoat as the system directs. If the holes remain as you level the surface, establish how far they run. Remove the defective material to a sound layer when the repair requires it, then rebuild the specified finish.
Before refinishing the piece, spray an equivalent scrap or sample panel. Copy the substrate and sealer, use the specified application and record what changed. Adjust only one approved variable at a time. Follow the SDS and local requirements for ventilation, ignition control and personal protection for solvent spray finishing.
Check the Gun Only After Checking the Process
If your lacquer calls for a 1.3 mm setup and you are choosing a gun, compare the PORPHIS PRD-817 VS. It is listed at about 15.2 CFM air consumption, so match gun airflow to compressor output and verify pressure under flow before buying. A correct setup helps you repeat the sample's application; it does not cure trapped solvent or contamination.
Questions About Lacquer Craters
Can I cover the holes with another coat
Adding material can leave the original defect intact or make drying harder. Identify the cause and follow the product's approved repair process before applying more finish.
Can the air hose cause craters if the part is clean
Yes, a contaminated line can affect wetting. Check the air at the point of use and work back through the hose, fittings and treatment system. Water or oil there is a problem to correct, not proof that a given crater came from trapped solvent.

Compartilhar:
Body Filler Showing Through Primer and How to Fix It